Product Data Sheet

Tenite Acetate 105E2R30025, Natural, Trsp

Application/Uses
  • Ophthalmics
  • Tool handles
  • Toys/Sporting goods
Product Description
Tenite cellulosic plastics are noted for their excellent balance of properties - toughness, hardness, strength, surface gloss, clarity, and a warm feel. The mechanical properties of Tenite cellulosic plastics differ with plasticizer levels. Lower plasticizer content yields a harder surface, higher heat resistance, greater rigidity, higher tensile strength, and better dimensional stability. Higher plasticizer content increases impact strength. Tenite cellulosic plastics are available in natural, clear, amber, and black. Color concentrates are available in let-down ratios from 10:1 to 40:1. Tenite Cellulose Acetate 105-25 is heat stabilized and has a plasticizer level of 25%.

Typical Properties
 
 
Plasticizer       25%
Specific Gravity     D 792  1.28 
 
Tensile Stress @ Yield     D 638  37.2 MPa (5400 psi)
Tensile Stress @ Break     D 638  40.7 MPa (5900 psi)
Elongation @ Break     D 638  25%
Flexural Modulus     D 790  2344 MPa (3.4 )
Flexural Yield Strength     D 790  62.7 MPa (9100 psi)
Rockwell Hardness, R Scale     D 785  90 
Izod Impact Strength, Notched 
  @ 23°C (73°F)
D 256  160 J/m (3.0 ft·lbf/in.)
  @ -40°C (-40°F)
D 256  48 J/m (0.9 ft·lbf/in.)
 
Deflection Temperature  d
  @ 1.82 MPa (264 psi)
D 648  77°C (171°F)
  @ 0.455 MPa (66 psi)
D 648  86°C (187°F)
Vicat Softening Temperature  d   D 1525  113°C (235°F)
 
Water Absorption, 24 h immersion     D 570  2.3%
Soluble Matter Loss     D 570  0.2%
Weight Loss on Heating   [72 hours @ 80°C (176°F)]  D 706  1.2%
 
     D 542  1.46-1.49 
Light Transmission  e   E 308  >90%
Haze  e   D 1003  <8.5%
Specific Heat   @ 23°C (73°F)  DSC  1.26-1.67 kJ/kg·K (0.301-0.399 Btu/lb·°F)
Thermal Conductivity     C 177  0.17-0.33 W/m·K (1.2-2.3 )
Coefficient of Linear Thermal Expansion     D 696  11- /°C (mm/mm·°C) (6- /°F (in./in.·°F))
Mold Shrinkage     D 955  0.2-0.6%
Dielectric Strength     D 149  11.8-18.7 kV/mm (300-475 V/mil)
Dielectric Constant   1 MHz  D 150  3.3-3.8 
Dissipation Factor   1 MHz  D 150  0.01-0.15 
Volume Resistivity     D 257  - ohm·cm
Characteristics
Formula 105 - heat stabilized.

Comments
Properties reported here are typical of average lots. Eastman makes no representation that the material in any particular shipment will conform exactly to the values given.